Magnet trading · Nike Industrial Trading[email protected]WhatsApp +852 4607 0157

Magnet materials and specifications

Hot-pressed vs sintered NdFeB magnets

For a block or arc, start with a sintered grade that meets your drawing and working conditions. Shortlist hot-deformed NdFeB when you need another orientation or more margin against hot demagnetization. For a radial ring, compare candidates by their field at the working gap.

Nike Industrial Trading Published 14 November 2026

Conceptual diagram contrasts field alignment before sintering with hot pressing followed by hot deformation
Schematic comparison of the material routes. Grain shapes and sizes are illustrative.

How hot pressing, hot deformation and sintering differ

If a quote says “hot pressed,” ask whether it covers the pressed blank or a finished magnet that has also been hot deformed. [1] [2] [3]

What the manufacturing route tells a buyer
Material or stageHow the easy axis is setWhat to verify
Hot-pressed compactHot pressing densifies the powder. In this two-step route the compact has little preferred magnetic orientation.Request finished-grade data if the quote only gives values for the compact.
Hot-deformed NdFeBDeformation aligns the grains and gives the magnet a preferred direction. Die upsetting and ring extrusion can produce different geometries and orientations.Specify the easy axis, field direction at the active surface and finished pole pattern.
Conventional sintered NdFeBA magnetic field aligns powder before sintering. The preferred direction carries through to the finished part.Check the grade, alignment direction, finish and drawing limits.

What the manufacturing route tells a buyer

Hot-pressed compact

How the easy axis is set
Hot pressing densifies the powder. In this two-step route the compact has little preferred magnetic orientation.
What to verify
Request finished-grade data if the quote only gives values for the compact.

Hot-deformed NdFeB

How the easy axis is set
Deformation aligns the grains and gives the magnet a preferred direction. Die upsetting and ring extrusion can produce different geometries and orientations.
What to verify
Specify the easy axis, field direction at the active surface and finished pole pattern.

Conventional sintered NdFeB

How the easy axis is set
A magnetic field aligns powder before sintering. The preferred direction carries through to the finished part.
What to verify
Check the grade, alignment direction, finish and drawing limits.

Grain texture describes the preferred material direction. The pole pattern describes the magnetized part. For a ring, specify both the orientation and the finished number and positions of poles. See magnetization directions and the ring drawing guide. [2] [4]

What changes after hot deformation?

In Ahn’s Dy-containing alloy, remanence rose from 0.793 to 1.339 T as the grains aligned during hot deformation. Intrinsic coercivity fell from 24.79 to 21.88 kOe in the same comparison between the blank and the hot-deformed specimen. [1]

Ahn et al., Tables 1 and 3. HP700 denotes the compact pressed at 700 °C. The second specimen was subsequently deformed at 785 °C at 0.019 mm/s.

Compare the finished grades’ remanence Br and intrinsic coercivity HcJ at the same temperature and along the same direction relative to the easy axis. Both are material properties. To check the field delivered by a drop-in replacement, measure at the specified working gap with the same assembly geometry, surrounding steel and probe direction. The normal B–H curve also provides the maximum energy product for material comparison. [1] [8]

What changes at 150 °C?

In Daido’s REPM 2025 comparison, the optimized hot-deformed sample, made without heavy rare-earth elements, had the lowest HcJ at 23 °C. At 150 °C it had the highest, exceeding the Dy-containing sintered sample by 72 kA/m and the Tb-containing sample by 52 kA/m. The three samples differ in composition as well as processing. [5]

Intrinsic coercivity (kA/m)
Sample23 °C150 °C
Hot-deformed, HRE-free1,725720
Sintered, with Dy1,873648
Sintered, with Tb1,935668

If the rotor magnets may reach 150 °C, hold any grade backed only by room-temperature data. A hot-deformed grade is worth testing if its hot curves show enough margin where the sintered option falls short. Use each grade’s normal B–H and intrinsic J–H curves at the actual magnet temperatures to check the local operating point closest to the knee across the relevant reverse-field conditions. [8]

Verify the required working-gap field or back-EMF under the specified duty. To check permanent loss, repeat the baseline measurement after cooling the magnet back to the original measurement temperature. Keep the fixture and measurement position fixed for a field test, or use the same speed for back-EMF. If the field falls below target, the knee margin is too small or permanent loss exceeds the limit, review the grade or design before comparing prices. See the PMSM demagnetization guide for hot and fault checks.

When is each route worth quoting?

For a block or arc, quote a known sintered grade first if it meets your drawing, required field and hot demagnetization limits. If it falls short, shortlist a hot-deformed grade when its orientation or hot curves address that gap. For a drop-in change, use the same part envelope and duty. In the Daido–Honda motor case the team changed the magnet shape and rotor, so the comparison was at motor level. [6] [7]

For a radial ring, ask which one-piece hot-deformed or radially oriented sintered designs can meet your dimensions. Compare them with a segmented assembly if your rotor permits one. Compare scans at the same working gap, field component, reference angle and axial planes. Set the minimum field per pole and the allowed pole-to-pole variation where they matter. [4] [11]

Huang’s team cut specimens from an experimental extruded ring and measured radial remanence of 0.85–0.86 T at the ends and 1.27–1.28 T in the middle. If the ends contribute to the working field in your design, check the finished ring against the field limit there as well as at the center. [10]

Compare cost per accepted assembly after the candidates meet the same field and fit requirements. For example, 1,000 accepted rotors with 12 segments each take 12,000 segments before yield losses. Add tooling and any finishing, magnetization, assembly or inspection costs outside the part quote. Divide the full lot cost by 1,000 and use the same accepted quantity for an integral ring.

Honda engineers made a C-shaped magnet by near-net sintering and by hot extrusion. Their extrusion process omitted grinding. Ask which finishing steps are included for your drawing. [6] [9]

What to send for a route comparison

For a replacement, send the existing drawing or part details and describe what needs to improve. For a new design without a drawing, send the space available, what the magnet must do and any known operating limits. Leave the grade and route open if you want options.

Part drawing, revision and available envelope:
Preferred direction and finished pole pattern:
Working magnet temperatures and reverse-field conditions, if known:
Field or flux target, measurement position and working gap:
Allowed permanent loss after hot duty, if specified:
Coating, fit and inspection requirements:
Prototype and production quantities:
Existing grade or curve, if available:

Related technical guides

Technical sources

Read each source with its stated material, test conditions and publication scope.

  1. Ahn et al. (2024), hot pressing and grain alignment
  2. Keszler et al. (2025), field-assisted consolidation and texture
  3. Cui et al. (2022), magnet manufacture, Part II
  4. Daido Electronics, anisotropic hot-deformed NdFeB
  5. Goto et al. (2025), REPM coercivity comparison
  6. Soma et al., C-shaped magnets in hybrid vehicles
  7. Daido Steel and Honda (2016), traction-motor case
  8. Shin-Etsu, N42SH data sheet and curves
  9. Yin and Constantinides, magnet manufacturing processes
  10. Huang et al. (2023), radial ring variation
  11. Ishimoto et al. (1996), radially oriented sintered rings

Need to compare two magnet routes?

Tell us what the current magnet falls short on or what the new design must achieve.

Compare magnet options