Magnet trading · Nike Industrial Trading[email protected]WhatsApp +852 4607 0157

Magnet materials and specifications

NdFeB remanence Br and N52 datasheet values

Br is the zero-internal-field intercept after saturation. An N52 value of 1.45 T can be typical, nominal or a catalog lower endpoint depending on the source. A gaussmeter reading on the part answers a different question.

Nike Industrial Trading Published 6 November 2026

K&J material remanence range versus the listed pole-center field for one N52 disc
K&J N52 material range compared with the catalog field of the D42-N52 disc. The readings have different test bases.

What remanence Br measures

Remanence, Br, is the flux density at zero internal magnetic field on the descending branch after the material has been saturated in the stated direction. Locate the H = 0 intercept on the normal B–H curve. In SI, B = μ0H + J, so the polarization J and flux density B coincide at that intercept. Br is reported in tesla, millitesla or gauss. [1] [5]

H = 0 here is a condition on the material curve. A loose magnet in air can have a reverse field inside it from its own poles even when the external field source is off. Its operating point depends on geometry and the surrounding magnetic circuit. See the guide to load lines and demagnetization curves to locate that point. [1] [6]

Schematic descending B and J branches coincide at internal H = 0. The axes are qualitative.

Is 1.45 T a valid N52 remanence?

Yes, when tied to the right source and value type. Arnold lists 1,450 mT, or 1.450 T, as typical Br for its N52 entry. K&J lists an N52 range of 14.5–14.8 kG, so 1.45 T is that table's lower endpoint. Shin-Etsu lists a different range for the specifically named N52-F. These entries answer different specification questions. [2] [3] [4]

Published remanence examples, not a merged grade specification
Source and designationBr (T)How it is listed
Arnold N521.450Typical
Arnold N52 data sheet1.420 / 1.450 / 1.480Min. / nominal / max. in rev. 210802
K&J N521.45–1.48Catalog range
Shin-Etsu N52-F1.41–1.47Range for the named material

For an acceptance limit of Br ≥ 1.45 T, Arnold's listed minimum and the lower end of the N52-F range are below the proposed limit. K&J's published lower endpoint equals the proposed limit. Arnold's plotted curves use nominal Br and minimum intrinsic coercivity. Use the agreed specification, sample method and reference temperature for acceptance of the offered material. [11]

“High remanence” needs a comparison basis. On K&J's own table, N42 has Br of 1.30–1.32 T versus N52 at 1.45–1.48 T. That is a material difference under the same catalog convention. Check the coercivity and temperature curves separately before replacing one material with the other. [3]

Use one unit before you compare documents: 1 T = 1,000 mT = 10,000 G = 10 kG. Thus 14.5 kG, 1,450 mT and 1.45 T can be the same value. Check that they are all in the Br column before comparing. The N52 numeral belongs to the maximum energy product convention. [5]

Why a gaussmeter can read much less than Br

A gaussmeter near a finished magnet reports a component of the local field at the sensor. Geometry, probe orientation, distance and nearby steel all change that reading. For example, K&J's finder lists 5,233 G of surface field for its D42-N52 disc at the pole center. Its separate material table lists N52 Br at 14,500–14,800 G. The difference is expected. Neither number should be substituted for the other. [3] [7] [8]

For a field acceptance test on an assembly, state the measurement point and orientation, probe offset, fixture, gap, temperature and limit. A part can meet a material Br requirement and still miss a field target because its pole pattern, geometry or installation differs. For a repeatable field procedure, see field strength and measurement.

What to compare on two test reports

  1. Match the material identity. Compare full grade and suffix, supplier specification revision, and whether the sample represents the finished magnetic material. Read the axis orientation, especially if the material has a preferred direction.
  2. Check the curve and field basis. Request the second quadrant and confirm the initial magnetization procedure, test temperature and whether H is the internal field. For an open-circuit measurement, ask how the self-demagnetizing field was corrected.
  3. Separate material and part criteria. Keep material Br, a lot or coupon result, and the completed part's field or flux test as different fields in the inspection record.

IEC 60404-5 describes methods for magnetic properties and demagnetization curves. IEC 60404-18 covers specified open magnetic circuit methods using a superconducting magnet and corrections for the specimen's self-demagnetizing field. Read the report's method before judging two intercepts side by side. [9] [10]

Material data enquiry checklist

If you have a drawing, an old part description or a field reading, send what you have and explain the result you need. Leave unknown items blank or mark them “unknown”. The first discussion can establish whether the requirement concerns material Br or the field at a point on the finished assembly, and which data would allow that comparison.

Drawing or existing part reference:
Named material grade and suffix:
Br minimum, typical or range, with units:
Test direction and reference temperature:
Manufacturer curve revision and test method:
Separate finished part field or flux requirement:

Technical sources

Read each source with its stated material, test conditions and publication scope.

  1. Arnold: Measuring magnetic properties
  2. Arnold: Neodymium grade table
  3. K&J: Neodymium material specifications
  4. Shin-Etsu: N series lineup
  5. NIST: Units for magnetic properties
  6. Lake Shore: Permanent magnet measurements with a VSM
  7. K&J: Disc magnet specifications
  8. K&J: Measuring magnets
  9. IEC 60404-5:2015: Permanent magnet measurements
  10. IEC 60404-18:2025: Open-circuit measurements
  11. Arnold: N52 individual data sheet, rev. 210802

Specifying a minimum remanence?

Send the grade data sheet or test report if you have one. A drawing, an existing part description or a field-reading problem can also start the discussion about which property needs checking.

Discuss a remanence requirement