Magnet trading · Nike Industrial Trading[email protected]WhatsApp +852 4607 0157

Magnet materials and specifications

Hot Pressing and Hot Deformation of NdFeB Magnets

Hot pressing makes a dense NdFeB blank. Subsequent deformation sets the preferred magnetic direction. Check that direction on the drawing, then compare finished-grade curves and field measurements at your working gap.

Nike Industrial Trading Published 20 November 2026

Heated tooling above a compact beside a plate and a radially oriented ring
Process schematic showing a compact, a plate and a ring after separate forming stages.

Hot pressing makes the blank. Deformation sets the direction.

In a common hot-deformation route, a melt-spinning wheel rapidly cools the alloy into thin ribbon. The ribbon is broken into powder flakes, then compacted under heat and pressure. The dense blank has little preferred magnetic direction. Deforming it at elevated temperature develops a grain texture, which gives the finished material an easy axis. [1] [3] [6]

Hot die upsetting reduces the blank’s height and can make a plate with an easy axis through its thickness. Backward extrusion forces material around a tool to form a ring with a radial easy axis. Put the required material direction on a section of the drawing and specify the finished pole pattern separately. A radially oriented ring can still require a particular pole count and angular reference at magnetization. [3] [6] See the magnetization direction guide and ring drawing guide.

Hot pressing densifies the flake powder. The deformation route sets the part geometry and preferred magnetic direction. Drawing is schematic. See Hioki Figure 3 and Chen et al.

How pressure, temperature and deformation affect the result

In Ahn and colleagues’ Dy-containing alloy, the HP700 compact was pressed at 700 °C. After hot deformation at 785 °C with a tool speed of 0.019 mm/s, its remanence rose from 0.793 to 1.339 T. Intrinsic coercivity fell from 24.79 to 21.88 kOe. It gained remanence and lost some resistance to a reverse field, so both properties matter when considering a replacement. [1]

Published examples of what the process can change
TrialWhat was comparedUse in a specification
Pressing pressure in a Ce-substituted alloyJeong et al. compared 100, 200 and 300 MPa at 700 °C, followed by the same hot deformation. The 200 and 300 MPa blanks both reached about 98% relative density. After deformation they gave 1.22 and 1.12 T in Br, and 8.9 and 8.2 kOe in intrinsic coercivity, respectively. [4]Check blank density for consolidation and use a finished-grade curve for magnetic acceptance.
Hot-deformation temperature in Hioki’s sample CAt a fixed strain and strain rate, the authors compared microstructure and demagnetization curves across deformation temperatures. The grains grew as the processing temperature rose in this series. [5]Ask for the finished grade and the curve at your working temperature. Keep the production temperature separate from the temperature of the magnetic test.

Published examples of what the process can change

Pressing pressure in a Ce-substituted alloy

What was compared
Jeong et al. compared 100, 200 and 300 MPa at 700 °C, followed by the same hot deformation. The 200 and 300 MPa blanks both reached about 98% relative density. After deformation they gave 1.22 and 1.12 T in Br, and 8.9 and 8.2 kOe in intrinsic coercivity, respectively. [4]
Use in a specification
Check blank density for consolidation and use a finished-grade curve for magnetic acceptance.

Hot-deformation temperature in Hioki’s sample C

What was compared
At a fixed strain and strain rate, the authors compared microstructure and demagnetization curves across deformation temperatures. The grains grew as the processing temperature rose in this series. [5]
Use in a specification
Ask for the finished grade and the curve at your working temperature. Keep the production temperature separate from the temperature of the magnetic test.

Tool speed in mm/s and strain rate in s−1 describe different quantities. A setup comparison needs the starting height and deformation history. For a component decision, start with Br, HcJ and the demagnetization curve of the actual grade. [1] [4] [7]

Where to check a backward-extruded ring

Huang and colleagues cut Ø2 × 2 mm samples from a ring with 20 mm outside diameter, 15 mm bore and 15 mm height. Using vibrating sample magnetometry, they measured radial remanence of 0.85–0.86 T at the ends and 1.27–1.28 T in the middle. If a design uses field near the ends, scan the finished magnetized ring at the working gap near both ends as well as at the midpoint. Use the same probe direction and angular datum at each height. [2]

Conceptual scan locations for a magnetized ring. The customer drawing sets the gap, field component and axial planes. Huang et al. measured cut material samples at different heights.

For a multipole ring, one example drawing note is “Scan the radial field at gap [g] and axial plane [z], with angle zero at [assembly datum] and positive radial field directed outward. At the designated pole center at zero, verify [expected sign]. Moving in [scan direction, viewed from the drawing’s reference face], verify [pole sequence] against the drawing. Within each pole sector record the peak absolute radial field. Each peak must exceed [minimum]. Calculate pole spread as 100 × (largest peak − smallest peak) / mean peak. Maximum spread: [percent].” Repeat at each specified plane. If the sensor reads at a fixed angle, specify the signed field at that angle and the positive probe direction. The route comparison covers when to shortlist a sintered alternative. The motor application guide takes the ring data into the assembly.

Details to send with a hot-deformed part inquiry

Finished shape, drawing revision and dimensions:
Preferred magnetization direction and pole pattern:
Working gap, field direction and axial measurement planes:
Magnet temperature and known reverse-field conditions:
Candidate grade or current part, if known:
Sample quantity and acceptance requirements:

Technical sources

Read each source with its stated material, test conditions and publication scope.

  1. Ahn et al., grain alignment in hot-deformed NdFeBTables 1 and 3 and Figure 9. Dy-containing laboratory samples.
  2. Huang et al., inhomogeneity in a backward-extruded ringSection 2 and Table 2. VSM results are for cut specimens.
  3. Hioki, hot-deformed NdFeB process and materialsSection 2 and Figure 3. Radial rings and axial plates.
  4. Jeong et al., hot-pressing pressure in Ce-substituted magnetsMethods, Table 1 and Figure 1. The hot-deformation condition was held fixed.
  5. Hioki et al., composition and hot-deformation temperatureTable 1 and Figures 1–2. Multiple sample compositions and temperatures.
  6. Chen et al., permanent magnets prepared by hot deformationSection 1 describes grain alignment and die upsetting versus backward extrusion.
  7. Keszler et al., field-assisted sintering and spark plasma texturingTable 3 distinguishes commercial hot deformation from the authors’ FAST/SPT experiments.

Specifying an oriented plate or radial ring?

Include the easy axis, finished poles and any field requirement at a specified gap.

Discuss a hot-deformed part