Magnet materials and specifications

How to read an NdFeB hysteresis loop

Read remanence at H = 0, normal coercivity where B = 0 and intrinsic coercivity where J = 0. Follow a worked teaching curve with tesla and kA/m axes, then check the sample and measurement conditions.

Nike Industrial Trading Published 5 November 2026

Initial magnetization curve and minor loop within a schematic major hysteresis loop
Separate conceptual magnetic histories on normalized axes. Not measured NdFeB data.

What an NdFeB hysteresis loop shows

A hysteresis loop records how a magnetic sample responds as the applied field is swept through a cycle. The return path differs from the outward path because the sample retains a magnetic history. NdFeB's substantial remanence and resistance to reversal make it useful as a permanent magnet; the complete loop shows more than the second-quadrant curve normally supplied for design.

To read one, identify the axis quantities, follow the chosen branch and record the intercepts with their units. The worked example below shows this process; the later sections explain why different measurement methods can change the interpretation.

Read Br, HcB and HcJ from one worked example

Teaching data, not a measured grade. This self-authored example assumes 20°C, field along the preferred magnetic axis and an internal-field H axis. The descending branch represents a return from assumed positive saturation. Its polarization points were chosen for instruction; B was calculated from B = μ₀H + J, with μ₀ ≈ 4π × 10−7 H/m.

Illustrative descending branch: Br = 1.20 T, HcB = 900 kA/m, HcJ = 1,600 kA/m. Assumed 20°C and internal H along the preferred axis. Synthetic teaching values, not measured grade data; B below the displayed window is included in the CSV.
  1. Read the axes. Horizontal H is in kA/m; the two vertical quantities B and J are in tesla. For B = μ₀H + J, convert kA/m to A/m first.
  2. Find H = 0 on the descending branch. Both curves meet at 1.20 T, giving Br = 1.20 T in this example.
  3. Follow B to zero. It crosses at H = −900 kA/m. Report the magnitude HcB = 900 kA/m; J is still about 1.131 T at that point.
  4. Follow J to zero. It crosses later, at H = −1,600 kA/m, giving HcJ = 1,600 kA/m. B is already negative there.
Results read from the teaching branch
QuantityResultWhere read
Br1.20 TH = 0
HcB900 kA/mB = 0
HcJ1,600 kA/mJ = 0

At H = −900 kA/m, the arithmetic is B ≈ (4π × 10−7 × −900,000) + 1.130973 = 0 T. The vanishing B therefore coexists with positive polarization. At H = −1,600 kA/m, J = 0 but B ≈ −2.011 T, below the plotted window. Download the illustrative branch points (CSV) to reproduce the calculation.

A real result should retain the sample ID, temperature, orientation, axis convention and measurement method alongside these three values. If the graph only says “field” or lacks a temperature, record that as missing; the teaching assumptions cannot fill it in. Grade identification and operating-temperature approval require the actual material data.

B–H, J–H and M–H: read the ordinate first

Three common material plots in SI units
PlotVertical axisRelationshipZero-crossing meaning
Normal B–H loopB in teslaB = μ₀H + JB = 0 on the descending branch identifies normal coercivity HcB
Intrinsic J–H loopJ in teslaJ = μ₀MJ = 0 identifies intrinsic coercivity HcJ
M–H loopM in A/mM = J / μ₀Its zero corresponds to intrinsic coercivity under the same measurement convention

Three common material plots in SI units

Normal B–H loop

Vertical axis
B in tesla
Relationship
B = μ₀H + J
Zero-crossing meaning
B = 0 on the descending branch identifies normal coercivity HcB

Intrinsic J–H loop

Vertical axis
J in tesla
Relationship
J = μ₀M
Zero-crossing meaning
J = 0 identifies intrinsic coercivity HcJ

M–H loop

Vertical axis
M in A/m
Relationship
M = J / μ₀
Zero-crossing meaning
Its zero corresponds to intrinsic coercivity under the same measurement convention

At the material condition H = 0, B and J coincide, so their remanent value is Br. HcB and HcJ are usually reported as positive magnitudes, although their descending-branch intercepts lie on the negative H axis. A normal B–H curve can cross B = 0 while the material still has substantial positive polarization; zero B does not mean zero magnetization.[1] [2]

A fourth format plots whole-sample moment m, in A·m² or emu. Dividing by magnetic material volume gives M only when that volume is known and the intended normalization is clear. A mass-normalized result needs density before it can be converted to volume magnetization. One emu of moment is 10⁻³ A·m².[2]

Check whether the horizontal axis is H in kA/m, H in oersted, or μ₀H in tesla. A field axis marked T often means μ₀H; it does not turn the graph into B–H. In air, 1 T of μ₀H corresponds to about 796 kA/m.

Major loop, minor loop and initial curve

Conceptual major loop on normalized axes. Arrows show the sweep direction; this diagram describes magnetic history rather than a measured material grade.

A major loop follows reversal between sufficiently high positive and negative fields. To interpret it as saturated behaviour, the measurement must reach a field adequate for that material, direction and temperature. Flattening caused by an instrument limit, processing or an incomplete sweep is not proof of saturation.

An initial magnetization curve starts from a specified demagnetized state and follows the first increase in field. It is not simply half of the major loop. State how the sample was prepared: its history affects the starting condition.

A minor loop reverses field before completing the major cycle. It describes the response around the states actually reached. A small recoil excursion used in a magnetic-circuit calculation is therefore different from reversing a magnet through both saturated states. Lake Shore's measurement examples distinguish initial, minor and major loops for NdFeB.[3]

The second-quadrant descending branch is the part used most often for operating-point calculations. For load lines, the knee and hot-state selection, continue to demagnetization curves and operating points.

Why two laboratories can report different curves

A closed-circuit hysteresisgraph places the specimen in a magnetic circuit and measures field and flux. Contact, alignment, sample thickness, instrumentation and calibration still affect the result. A vibrating-sample magnetometer (VSM) measures sample moment in an applied field, normally with an open specimen geometry.[4]

For an open specimen, the field inside the material differs from the applied field because of its demagnetizing field. Under a uniform-magnetization ellipsoid approximation in SI, Hinternal = Happlied − NM, with a dimensionless demagnetizing factor N. Non-ellipsoidal parts can have nonuniform internal fields; one scalar correction may only approximate them. CGS conventions place factors differently, so copy neither the equation nor a factor table without its unit convention.[5]

Consequently, “remanence at zero applied field” from an uncorrected open-sample measurement is not automatically the same material Br read at internal H = 0. This distinction matters when comparing a VSM plot with a manufacturer's closed-circuit datasheet.

Sample shape can also change coupling to a VSM's pickup coils and affect moment calibration. That instrument correction is separate from correcting internal field for demagnetization. Mixing the two can leave an apparently tidy but incorrectly scaled curve.[6]

Before treating a small offset or a branch asymmetry as material behaviour, review sample orientation, centring, background subtraction, drift, field settling and sweep history. Research measurement guidance shows why processing and instrumental artefacts need checking alongside the plotted curve.[7]

Loop area, energy loss and BHmax

For a consistent scalar B–H loop under the stated cyclic conditions, the magnitude of ∮H dB gives the energy dissipated per unit volume per cycle, in J/m³. On an M–H plot, the corresponding integral needs the factor μ₀. Whole-sample moment and μ₀H axes instead give energy per sample, before division by volume.

This loop area is not (BH)max. Maximum energy product is the largest magnitude of B × H in the second quadrant of the normal curve. It is a rectangle-based material figure of merit, not the enclosed full-loop area.

A stationary permanent magnet does not continuously dissipate the full-loop energy simply by holding an object. The loss applies when the magnetic state undergoes the stated cycle. Multiplying by frequency requires that the relevant loop and losses correspond to that cycling condition; a quasistatic curve alone is not a complete high-frequency loss prediction.[8]

What to request with a hysteresis graph

Material / grade, sample ID and magnetic history:
Sample dimensions, mass and magnetic material volume:
Orientation of the field relative to the preferred axis:
Temperature and stabilization method:
Instrument and open / closed circuit arrangement:
Axis quantities, units and normalization:
Applied-field range, sweep direction / rate and saturation check:
Demagnetizing correction and moment-calibration method:
Raw numeric data, processing notes and uncertainty:

Numeric data are more useful than a screenshot when extracting intercepts or checking a model. Keep the measurement conditions with the file. If the maximum field was insufficient for a full major loop, label the result accordingly rather than presenting it as a saturated material certificate.

Send the labelled graph and the component question even if you do not have every item above. We can help identify the values and missing document details to clarify with the proposed supply. A graph with unknown axes or sample conditions needs those gaps resolved before it becomes an acceptance requirement.

Related measurements and applications

Technical sources

Read each source with its stated material, test conditions and publication scope.

  1. Dexter / Allegro: The science of magnets
  2. NIST: Magnetic units conversion chart
  3. Lake Shore: VSM materials and measurement examples
  4. Arnold: Magnetic properties and measuring techniques
  5. Lake Shore: Measurements with a VSM: permanent magnet materials
  6. Quantum Design: Reported moment: sample shape effects
  7. Paterson et al. / AGU: Measuring, processing and analyzing hysteresis data
  8. MIT: Electromagnetic Fields and Energy, 11.5

Need to interpret a material curve?

Send the labelled graph and the component question. We can help identify the values and missing document details to clarify with the proposed supply.

Discuss magnetic data