What is the Brinell hardness of NdFeB magnets?
The sintered NdFeB data sheets examined here report Vickers hardness. Shin-Etsu lists 600 HV for N36SH and Arnold lists 620 HV in its N52 catalog sheet. These documents do not establish a Brinell value for either material. For an HBW requirement, first ask the laboratory whether the method applies and whether the available specimen can produce a valid impression. Agree on representative material and test conditions before using the result.[1] [3] [5]
Brinell uses a ball and measures the diameter of the residual impression. Vickers uses a diamond pyramid and measures both diagonals. Material-specific conversion tables, such as the ones ASTM E140 publishes for specified metal families, are approximate. A table for steel cannot establish an HBW acceptance limit for sintered NdFeB. Also check whether a search result describes the element neodymium or the finished NdFeB alloy.[1] [2]
Read the Vickers value with its test conditions
| Source and material | Vickers value | What the table establishes |
|---|---|---|
| Shin-Etsu N36SH [3] | 600 HV | Grade-sheet reference. The sheet describes its values as non-standard. |
| Neorem sintered NdFeB [4] | 600 HV | Characteristic value at 20°C. No individual grade is specified. |
| Arnold N52 [5] | 620 HV | Catalog example for this grade. The hardness row has no load designation. |
| Goudsmit N40 [6] | 500–700 HV | Typical range in the 20°C mechanical properties table. |
These rows give a useful scale for reading a data sheet. They do not establish a hardness ranking between N36SH and N52. For a direct comparison, check the load and dwell, surface preparation, material lot, and the tested face relative to the alignment axis. A value labeled only “600 HV” is incomplete for duplicating a test.
A study on one sintered Dy-doped NdFeB material gives a more controlled comparison. With a 2.94 N load and 10 s dwell, the researchers measured 613.2 HV before the aging treatment and 561.8 HV after it. The study also found higher intrinsic coercivity after aging. This is a documented trade-off in those samples, with no implied trend across commercial magnetic grade numbers.[7]
Calculate a Vickers reading from the diagonals
After unloading, measure the two diagonals of the impression and average them. In the conventional HV number calculation, HV = 1.8544 × F / d², with load F in kgf and mean diagonal d in mm. If the machine gives force in newtons, divide by 9.80665 N/kgf before using that form of the equation.[8]
For a hypothetical polished coupon, suppose a 1 kgf load held for 12 s leaves diagonals of 55.0 and 56.2 μm. Then d = 55.6 μm = 0.0556 mm, and 1.8544 × 1 / 0.0556² ≈ 600 HV 1. The 1 denotes the load in kgf. Record the dwell time and specimen details with the result. An indistinct corner or a damaged impression needs review before its diagonals are used.
Separate the surface layer from the magnet body
State which layer you want to characterize. A deep indent on a thin coating can include a response from the substrate. For a substrate comparison, agree on a bare surface or a representative uncoated coupon from the same material and process. For a coating comparison, agree on the measurement geometry and how the method limits substrate influence. A NIST thin-film study illustrates why the indenter depth and underlying material both matter to the result.[9]
Hardness measures resistance to indentation. Edge chipping and breakage depend on how cracks initiate and grow under the actual load. NIST distinguishes cracks made by a Vickers impression from the controlled crack geometry used in standardized fracture-toughness tests. If the issue is chipped edges on finished parts, agree on an edge-break or chip allowance and inspect the finished parts after the operation under investigation. For a loaded assembly, use the strength and fracture guide to identify the relevant test.[10]
What to put on a hardness request
If a legacy drawing says “600 hardness,” ask its owner to confirm the scale before using the number as a limit. If the goal is to compare material lots, request the same method and specimen condition from each supplier and separate typical values from acceptance criteria. The dimensions and inspection guide covers the separate finished-edge check.
Drawing or part reference and material route: Property required: substrate HV, coating hardness, or direct HBW: Test load, dwell, method and acceptance limits: Test face, surface condition and coating thickness if relevant: Representative coupon or finished part and lot traceability: Edge damage or fit problem the result should help evaluate:
Technical sources
Read each source with its stated material, test conditions and publication scope.
- NIST: indentation hardness methods
- ASTM E140: public scope and limits of hardness conversion
- Shin-Etsu N36SH material sheet
- Neorem: characteristic properties of sintered NdFeB
- Arnold: sintered NdFeB catalog, N52
- Goudsmit: N40 datasheet in the NdFeB grade system
- Wang et al.: aging and mechanical properties of sintered Dy-doped NdFeB
- NIST SRM 2831: Vickers calibration and calculation
- NISTIR 5313: film and substrate effects in indentation
- NIST: critical review of the Vickers indentation crack method